Material Properties Titanium AlloyTi-6Al-2Nb-1Ta-0.8Mo As-Rolled admin May 20, 2016 Material Properties for Titanium AlloyTi-6Al-2Nb-1Ta-0.8Mo As-Rolled Physical specifications of materials. Materials Titanium AlloyTi-6Al-2Nb-1Ta-0.8Mo Description As-Rolled Density g/cc 4.48 lb/in^3 0.162 Hardness Brinell unless specified 290 Tensile Strength ultimate Mpa 830 Ksi 120.35 Yield Strength MPa 760 Ksi 110.2 Modulus of Elasticity Gpa 117 10^6 Psi 16.956521712 Poisson’s Ratio 0.31 %Elongation at break 10 %Reduction of area 28 Izod Impact J Ft-lb Fracture Toughness Mpa(m)^0.5 Ksi(in)^0.5 Thermal conductivity W/m-K 6.4 Btu/ft-h-F 3.6994219648 Specific Heat Cpacity J/g-K 0.552 Btu/lb-F 0.13248 Coefficient of thermal expansion 1E-6/K 9.2 1E-6/F 5.1187969884 Electrical Resistivity Ohm-cm 0.00016