Material Properties

Stainless Steel 17-7 PH Cold Rolled

Material Properties for Stainless Steel 17-7 PH Cold Rolled

Physical specifications of materials.

Materials Stainless Steel 17-7 PH
  Description Cold Rolled
Density g/cc 7.8
  lb/in^3 0.282
Hardness Brinell unless specified 378
Tensile Strength ultimate Mpa 1380
  Ksi 200.1
Yield Strength MPa 1210
  Ksi 175.45
Modulus of Elasticity Gpa 204
  10^6 Psi 29.565217344
Poisson’s Ratio   0.27
%Elongation at break 1
%Reduction of area
Izod Impact J
  Ft-lb
Fracture Toughness Mpa(m)^0.5
  Ksi(in)^0.5
Thermal conductivity W/m-K 16.4
  Btu/ft-h-F 9.4797687848
Specific Heat Cpacity J/g-K 0.46
  Btu/lb-F 0.1104
Coefficient of thermal expansion 1E-6/K 11
  1E-6/F 6.120300747
Electrical Resistivity Ohm-cm 0.000083