Material Properties

Electrolytic tough pitch Copper, (C11000) Cold Worked

Material Properties for Electrolytic tough pitch Copper, (C11000) Cold Worked

Physical specifications of materials.

Materials Electrolytic tough pitch Copper, (C11000)
  Description Cold Worked
Density g/cc 8.89
  lb/in^3 0.321
Hardness Brinell unless specified 95
Tensile Strength ultimate Mpa 345
  Ksi 50.025
Yield Strength MPa 310
  Ksi 44.95
Modulus of Elasticity Gpa 122
  10^6 Psi 17.681159392
Poisson’s Ratio   0.33
%Elongation at break 12
%Reduction of area
Izod Impact J
  Ft-lb
Fracture Toughness Mpa(m)^0.5
  Ksi(in)^0.5
Thermal conductivity W/m-K 388
  Btu/ft-h-F 224.277456616
Specific Heat Cpacity J/g-K 0.385
  Btu/lb-F 0.0924
Coefficient of thermal expansion 1E-6/K 17
  1E-6/F 9.458646609